牌号 A2
对应标准 BS 3100-1991
一般工程用铸钢件
Specification for Steel castings for general engineering purposes
归类 铸钢
标签 碳钢铸钢
A2 化学元素成分含量(%)
成分 C Si Mn P S
最小值 - - - - -
最大值 0.35 0.6 1 0.05 0.05
①碳含量每降低0.01%,最大锰含量则增加0.04%,允许最大锰含量到1.1%
A2 机械性能
热处理或状态
抗拉强度
σb
Mpa
屈服点
σs
Mpa
断后伸长率或延伸率
δ
%
冲击吸收能量
KV2
J
A或N或N+T或OQ+T或WQ+T ≥490 ≥260 ≥18 ≥20
A=for anneal by heating to a temperature above the AC3 and cool in the furnace
N=for normalize by heating to a temperature above the AC3 and cool in still air
OQ=for quench into oil from a temperature above the AC3
WQ=for quench into water from a temperature above the AC3
AH=for air harden by heating to a temperature above the AC3 and cool in air at a rate fast enough to produce a hardened microstructure
T=for temper by heating to a temperature below AC1
ST=for solution treat by heating to temperature high enough to dissolve and any intermetallic phases followed by a rapid cool.
①表中值适用于铸件截面厚度小于等于500mm,超过此尺寸的机械性能应与制造商协商。
②如果买方要求对此牌号进行冲击试验,则不进行弯曲试验
近似对照表 铸钢
中国 日本 美国 国际标准组织 德国 俄罗斯 英国
GB JIS UNS ISO DIN EN/DIN W-Nr. GOST BS EN/BS
ZG270-500 SC480 J04000 270-480 GS-60
GS-62
1.0553
1.0555
35Л A2
A2 对应不同标准
1 GB /T 700-2006 碳素结构钢
2 ASTM A681-2008(R2015) 合金工具钢标准规范
3 GB /T 3274-2017 碳素结构钢和低合金结构钢热轧钢板和钢带
4 BS 3100-1991 一般工程用铸钢件
A2