位置: 网站首页 材料
牌号 2205 HS
美国UNS S32205 HS
对应标准 ASTM A313/A313M-2018
不锈钢弹簧丝
Stainless Steel Spring Wire
归类 双相不锈钢
标签 奥氏体-铁素体
说明 “HS”高强度
本标准适用于制造弹簧的奥氏体、奥氏体-铁素体、沉淀硬化不锈钢圆钢丝。
2205 HS 化学元素成分含量(%)
成分 C Si Mn P S Cr Ni Mo N
最小值 - - - - - 22 4.5 3 0.14
最大值 0.03 1 2 0.03 0.02 23 6.5 3.5 0.2
2205 HS 机械性能
直径
d
mm
抗拉强度
σb
Mpa
0.2≤d≤0.7 2370~2730
0.7<d≤0.8 2230~2570
0.8<d≤1 2140~2460
1<d≤1.5 2090~2410
1.5<d≤2 2000~2300
2<d≤2.5 1910~2190
2.5<d≤3 1860~2140
3<d≤3.5 1810~2090
3.5<d≤4 1770~2030
4<d≤4.5 1720~1980
4.5<d≤5 1670~1930
注:Tensile requirements for high strength cold drawn, as-delivered wire. Tensile strength can be increased by 29 ksi [200 MPa] up to 65 ksi [450 MPa] by tempering depending on tensile and tempering conditions. Recommendations: 840°F [450℃]/1~3 h for batch tempering; 950°F [500°C] for 3 to 10 minutes in a continuous conveyor furnace. Shorter times may result in uneven tempering.
During storage, the tensile strength will increase somewhat due to aging. Depending on the storage conditions, the tensile strength can Increase by 0~12ksi [0~80 MPa].
注:数据仅供参考!如有疑问,请填写"我要纠错"!