位置: 网站首页 材料
牌号 425C12
对应标准 BS 3100-1991
一般工程用铸钢件
Specification for Steel castings for general engineering purposes
归类 铸钢
性能 耐腐蚀
标签 不锈钢铸钢
425C12 化学元素成分含量(%)
成分 C Si Mn P S Cr Ni Mo
最小值 - - - - - 11.5 3.5 0.4
最大值 0.06 1 1 0.04 0.03 14 4.5 1
425C12 机械性能
热处理或状态
抗拉强度
σb
Mpa
屈服点
σs
Mpa
断后伸长率或延伸率
δ
%
≥755 ≥550 ≥15
A=for anneal by heating to a temperature above the AC3 and cool in the furnace
N=for normalize by heating to a temperature above the AC3 and cool in still air
OQ=for quench into oil from a temperature above the AC3
WQ=for quench into water from a temperature above the AC3
AH=for air harden by heating to a temperature above the AC3 and cool in air at a rate fast enough to produce a hardened microstructure
T=for temper by heating to a temperature below AC1
ST=for solution treat by heating to temperature high enough to dissolve and any intermetallic phases followed by a rapid cool.
①AH或OQ(from 950°C to 1050°C)+T(590°C to 650°C)或AH或OQ(from 950°C to 1050°C), T(660°C to 700°C) and cool in air to below 95°C and T(590°C to 620°C)
近似对照表 耐蚀铸钢(不锈钢铸件)
中国 中国台湾 日本 韩国 美国 国际标准组织 德国 法国 俄罗斯 英国
GB ISC CNS JIS KS ASTM UNS ISO DIN EN/DIN W-Nr. NF EN/NF GOST BS EN/BS
ZG06Cr12Ni4 C54860 SCS 6 SCS 6X SSC 6 CA6NM J91540 GX4CrNi12-4 GX4CrNi13-4 1.4317 GX4CrNi13-4 08Х14Н7МЛ 425C12
注:数据仅供参考!如有疑问,请填写"我要纠错"!